Mechanical
Yield strengthnot given (tensile used)
Ultimate tensile strength140MPasourcestress at break, 23 °C
Flexural strength210MPasourcetypical, 23 °C
Elongation at break3%sourcestrain at break, 23 °C
Young's modulus (stiffness)9.8GPasourcetypical, 23 °C
Density1,530kg/m³sourcetypical
Strength to weight91.5kN·m/kg
Stiffness to weight6.41MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound2,531m/s
Thermal
Thermal conductivity0.27W/m·Ksourcetypical (DIN 52612-1)
Thermal expansion25µm/m·Ksourcelongitudinal (flow), mean 23-55 °C
100 mm part over a 50 °C swing125µm growth
Specific heat1,050J/kg·Ksourcetypical, 23 °C
Heats up and cools (diffusivity)0.168mm²/s
Thermal shock resistancenot sourced
Melting point223°CsourceDSC (ISO 11357)
Max service temperature205°CsourceHDT 1.8 MPa
Values forBASF Ultradur B 4300 G6 (PBT, 30% glass fibre), injection moulding grade; product information sheet 09/2026, typical values for uncoloured product at 23 °C.

Among 72 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PPS GF40Plastic LCP GF30Plastic PBT GF30
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PPS GF40Plastic LCP GF30Plastic PBT GF30
Strength against density

Compare Plastic PBT GF30 with