Materials / Compare

Plastic PEEK vs. Plywood

Compare Plastic PEEK vs. Plywood strength, stiffness, weight and thermal properties.

Change either side
Plastic PEEKBulk polymer (molded or machined)
PlywoodNatural
Try it on a partA sample part to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strength98MPasourcetypical, tensile yieldnot given (tensile used)
Ultimate tensile strengthnot sourced41.4MPasourcemodulus of rupture (no direct tensile value)
Compressive strength125MPasourcetypical, 23 Cnot sourced
Flexural strength165MPasourcetypical, flexural stress at yield, 23 C41.4MPasourcestatic bending MOR (Douglas-fir); range 33.72-42.61 across species
Elongation at break25%sourcetypical, at breaknot sourced
Young's modulus (stiffness)4GPasourcetypical (nominal)7.45GPasourcestatic bending MOE of the panel (Douglas-fir); range 6.96-8.55 across species
Density1,300kg/m³sourcetypical (crystalline)not sourced
Strength to weight75.4kN·m/kgnot sourced
Stiffness to weight3.08MN·m/kgnot sourced
Poisson's ratio0.38sourcetypicalnot sourced
Shear modulus1.45GPanot sourced
Bulk modulus5.56GPanot sourced
Speed of sound1,754m/snot sourced
Thermal
Thermal conductivity0.29W/m·Ksourcetypical, average, 23 C0.12W/m·KsourceAPA-recommended design value (Douglas-fir plywood), as reported by FPL/ORNL
Thermal expansion55µm/m·Ksourceaverage of flow/cross-flow, below Tg (<143 C)3.1–4.5µm/m·Ksourcebase material: solid wood parallel to grain, ovendry, range across species
100 mm part over a 50 °C swing275µm growth19µm growth14.5x less
Specific heat2,200J/kg·Ksourcetypical, 23 °C, DSC (Victrex PEEK 450G TDS, revision Jul 2012)1,700J/kg·Ksourcebase material: solid wood (all species), 12% MC, 27 C
Heats up and cools (diffusivity)0.101mm²/snot sourced
Thermal shock resistance80.1W/mnot sourced
Melting point343°Csourcetypical, DSCnot sourced
Glass transition143°Csourceonset (midpoint 150 C)not sourced
Max service temperature240°CsourceUL 746B RTI, mechanical strength (continuous use index)not sourced
Values forVictrex PEEK 450G (unreinforced, injection moulded), Victrex TDS rev. March 2026; Poisson from Victrex fluid-management flyer (2020-07)Douglas-fir plywood sheathing (construction plywood per PS 1), static bending properties from USDA FPL Wood Handbook FPL-GTR-282 Ch. 12 Table 12-2 (Biblis 2000)

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Is Plastic PEEK stronger than Plywood?

Plastic PEEK is stronger: its yield strength is 98 MPa against tensile strength 41.4 MPa for Plywood (2.37x).

Which is stiffer, Plastic PEEK or Plywood?

Plywood is stiffer: Young's modulus 7.45 GPa against 4 GPa for Plastic PEEK, so the same part in Plywood deflects less under the same load.

Which conducts heat better, Plastic PEEK or Plywood?

Plastic PEEK conducts heat better: 0.29 W/m·K against 0.12 W/m·K for Plywood.

Which expands less with temperature?

Plywood expands less: 3.8 µm/m·K against 55 µm/m·K for Plastic PEEK.

Among 72 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PEEK
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PEEK
Strength against density

Related comparisons