Materials / Compare

Plastic PMMA vs. SLA Resin Standard

Compare Plastic PMMA vs. SLA Resin Standard strength, stiffness, weight and thermal properties.

Change either side
Plastic PMMABulk polymer (molded or machined)
SLA Resin Standard3D printed (SLA resin)
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strengthnot given (tensile used)not given (tensile used)
Ultimate tensile strength80MPasourcetypical, 23 °C60MPasourcetypical
Compressive strength110MPasourcecompressive yield stress, typicalnot sourced
Flexural strength115MPasourcetypical105MPasourcetypical
Elongation at break5.5%sourcetypical8%sourcetypical45% more ductile
Young's modulus (stiffness)3.3GPasourcetypical, short-term2.75GPasourcetypical
Density1,190kg/m³sourcetypicalnot sourced
Strength to weight67.2kN·m/kgnot sourced
Stiffness to weight2.77MN·m/kgnot sourced
Poisson's ratio0.37sourcetypicalnot sourced
Shear modulus1.2GPanot sourced
Bulk modulus4.23GPanot sourced
Speed of sound1,665m/snot sourced
Thermal
Thermal conductivity0.19W/m·Ksourcetypicalnot sourced
Thermal expansion70µm/m·Ksource0-50 °Cnot sourced
100 mm part over a 50 °C swing350µm growthnot sourced
Specific heat1,470J/kg·Ksourcetypicalnot sourced
Heats up and cools (diffusivity)0.109mm²/snot sourced
Thermal shock resistance41.5W/mnot sourced
Max service temperature80°Csourcemax. permanent service temperature59°CsourceHDT 1.8 MPa
Values forRöhm PLEXIGLAS GS 0F00 cast acrylic sheet, typical values at 23 °C / 50 % RH (Röhm Technical Information Ref. No. 211-1)Formlabs Clear Resin V5 (FLGPCL05), TDS Rev. 01 March 20, 2024; printed on Form 4 at 100 µm, washed 5 min in >=99% IPA, post-cured 15 min at 60 °C in Form Cure. Orientation not stated.

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Standard is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Is Plastic PMMA stronger than SLA Resin Standard?

Plastic PMMA is stronger: its tensile strength is 80 MPa against 60 MPa for SLA Resin Standard (33%).

Which is stiffer, Plastic PMMA or SLA Resin Standard?

Plastic PMMA is stiffer: Young's modulus 3.3 GPa against 2.75 GPa for SLA Resin Standard, so the same part in Plastic PMMA deflects less under the same load.

Which is more ductile, Plastic PMMA or SLA Resin Standard?

SLA Resin Standard stretches further before it breaks: 8% elongation at break against 5.5% for Plastic PMMA.

Among 72 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropyleneFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PMMA
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropyleneFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PMMA
Strength against density

Related comparisons