Materials / Plastic

Plastic PMMA

Plastic PMMA (Acrylic) strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic PMMA, smooth finish.

ProcessBulk polymer (molded or machined)
Mechanical
Yield strengthnot given (tensile used)
Ultimate tensile strength80MPasourcetypical, 23 °C
Compressive strength110MPasourcecompressive yield stress, typical
Flexural strength115MPasourcetypical
Elongation at break5.5%sourcetypical
Young's modulus (stiffness)3.3GPasourcetypical, short-term
Density1,190kg/m³sourcetypical
Strength to weight67.2kN·m/kg
Stiffness to weight2.77MN·m/kg
Poisson's ratio0.37sourcetypical
Shear modulus1.2GPa
Bulk modulus4.23GPa
Speed of sound1,665m/s
Thermal
Thermal conductivity0.19W/m·Ksourcetypical
Thermal expansion70µm/m·Ksource0-50 °C
100 mm part over a 50 °C swing350µm growth
Specific heat1,470J/kg·Ksourcetypical
Heats up and cools (diffusivity)0.109mm²/s
Thermal shock resistance41.5W/m
Max service temperature80°Csourcemax. permanent service temperature
Values forRöhm PLEXIGLAS GS 0F00 cast acrylic sheet, typical values at 23 °C / 50 % RH (Röhm Technical Information Ref. No. 211-1)

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropyleneFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic PMMA
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropyleneFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic PMMA
Strength against density