MechanicalPlastic POM/AcetalStainless Steel 17-4PH
Yield strength69MPa11,275MPa218.5x stronger
Ultimate tensile strength69MPa11,379MPa220x stronger
Compressive strength124MPa1not sourced
Flexural strength99MPa1not sourced
Elongation at break75%18.33x more ductile9%2
Young's modulus (stiffness)2.8GPa1H 900197GPa270.4x stiffer
Density1,420kg/m³35.49x lighterH 9007,800kg/m³2
Strength to weight48.6kN·m/kg163kN·m/kg3.36x higher
Stiffness to weight1.97MN·m/kg25.3MN·m/kg12.8x higher
Poisson's ratio0.351H 9000.2722
Shear modulus1.04GPa77.4GPa74.7x stiffer in shear
Bulk modulus3.11GPa144GPa46.3x higher
Speed of sound1,404m/s5,026m/s3.58x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalStainless Steel 17-4PH
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalStainless Steel 17-4PH
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic POM/AcetalStainless Steel 17-4PH
Thermal conductivity0.4W/m·K1at 149 °C17.9W/m·K244.7x more heat through a fin
Thermal expansionmean122µm/m·K1mean10.8µm/m·K211.3x less
100 mm part over a 50 °C swing610µm growth54µm growth11.3x less
Specific heataverage -18 to 100 °C1,465J/kg·K13.18x highermean460J/kg·K2
Heats up and cools (diffusivity)0.192mm²/s4.99mm²/s25.9x faster
Thermal shock resistance52.5W/m7,809W/m149x more resistant
Melting point175°C1not sourced
Max service temperatureHDT 1.8 MPa125°C1316°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalStainless Steel 17-4PH
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalStainless Steel 17-4PH
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: DuPont, Cleveland-Cliffs
Plastic POM/Acetal
DuPont Delrin 100 acetal homopolymer, Table 2 'Typical Properties of Delrin Acetal Resins' (ASTM methods), Delrin Design Guide Module III hosted on delrin.com
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
  1. 1
    Delrin Acetal Resin Design Guide, Module IIIDuPontarchived copyPlastic POM/Acetal · Yield strength: typical (single ASTM D638 tensile strength)Plastic POM/Acetal · Ultimate tensile strength: typicalPlastic POM/Acetal · Compressive strength: compressive stress at 10% deformationPlastic POM/Acetal · Flexural strength: flexural yield strength, typicalPlastic POM/Acetal · Elongation at break: typicalPlastic POM/Acetal · Young's modulus (stiffness): typicalPlastic POM/Acetal · Poisson's ratio: typicalPlastic POM/Acetal · Thermal conductivity: typicalPlastic POM/Acetal · Thermal expansion: mean, 29 to 60 °CPlastic POM/Acetal · Specific heat: average -18 to 100 °C, Delrin acetal resins (not grade-specific)Plastic POM/Acetal · Melting point: crystalline melting pointPlastic POM/Acetal · Max service temperature: HDT 1.8 MPa (annealed)
  2. 2
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
  3. 3
    Delrin 100 Product Data SheetDuPontPlastic POM/Acetal · Density: typical (DuPont product information for Delrin 100 NC010; 'The data listed here fall within the normal range of product properties')

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plastic POM/Acetal stronger than Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 69 MPa for Plastic POM/Acetal (18.5x).

Which is lighter, Plastic POM/Acetal or Stainless Steel 17-4PH?

Plastic POM/Acetal is lighter: 1,420 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.

Which is stiffer, Plastic POM/Acetal or Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 2.8 GPa for Plastic POM/Acetal, so the same part in Stainless Steel 17-4PH deflects less under the same load.

Which is lighter for the same job, Plastic POM/Acetal or Stainless Steel 17-4PH?

For the same stiffness or strength: Plastic POM/Acetal is lighter for a stiff panel or plate, strong panel or plate; Stainless Steel 17-4PH is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam.

Part that must bePlastic POM/AcetalStainless Steel 17-4PH
Stiff rod or tie (tension)12.8x heavierlighter
Stiff beam (bending)1.53x heavierlighter
Stiff panel or platelighter33% heavier
Strong rod or tie3.36x heavierlighter
Strong beam27% heavierlighter
Strong panel or platelighter28% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic POM/Acetal or Stainless Steel 17-4PH?

Plastic POM/Acetal stretches further before it breaks: 75% elongation at break against 9% for Stainless Steel 17-4PH.

Thermal

Which conducts heat better, Plastic POM/Acetal or Stainless Steel 17-4PH?

Stainless Steel 17-4PH conducts heat better: 17.9 W/m·K against 0.4 W/m·K for Plastic POM/Acetal.

Which expands less with temperature?

Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 122 µm/m·K for Plastic POM/Acetal.