Nickel Inconel 718 (annealed + aged) strength, stiffness, density and thermal properties, with their source.

A bracket in Nickel Inconel 718, brushed finish.

ProcessWrought
Mechanical
Yield strength1,207MPasourcetypical, 1.0 in. hot-rolled bar, 0.2% offset
Ultimate tensile strength1,389MPasourcetypical, 1.0 in. bar
Elongation at break20%sourcetypical, 1.0 in. bar
Young's modulus (stiffness)200GPasourcetypical, 21 °C, annealed + aged
Density8,221kg/m³sourcenominal, annealed and aged
Strength to weight147kN·m/kg
Stiffness to weight24.3MN·m/kg
Poisson's ratio0.294sourcetypical, 21 °C, annealed + aged
Shear modulus77.3GPa
Bulk modulus162GPa
Speed of sound4,932m/s
Thermal
Thermal conductivity11.4W/m·Ksourcetypical, 21 °C, annealed + aged (calculated from resistivity per footnote a)
Thermal expansion13.2µm/m·Ksourcetypical, mean 21-93 °C, annealed + aged
100 mm part over a 50 °C swing66µm growth
Specific heat435J/kg·Ksourcetypical, 21 °C
Heats up and cools (diffusivity)3.19mm²/s
Thermal shock resistance3,680W/m
Melting point1,260–1,336°Csourcemelting range
Max service temperature704°Csourceupper use temperature stated by producer
Values forINCONEL alloy 718, standard grade, 1750 °F/1 hr anneal + 1325 °F/8 hr F.C. to 1150 °F aged; Special Metals bulletin SMC-045 typical values

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelNickel Inconel 718
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickNickel Inconel 718
Strength against density

Compare Nickel Inconel 718 with