Materials / Compare

Aluminum 6061-T6 vs. FDM Polycarbonate

Compare Aluminum 6061-T6 vs. FDM Polycarbonate strength, stiffness, weight and thermal properties.

Aluminum 6061-T6Wrought
FDM Polycarbonate3D printed (FDM)
MechanicalAluminum 6061-T6FDM Polycarbonate
Yield strength276MPa15.18x stronger53.3MPa2
Ultimate tensile strength310MPa15.82x stronger53.3MPa2
Flexural strengthnot sourced89.4MPa2
Elongation at break17%11.85x more ductile9.2%2
Young's modulus (stiffness)68.3GPa128.5x stiffer2.39GPa2
Density2,700kg/m³1range1,180–1,200kg/m³2
Strength to weight102kN·m/kg2.28x higher44.8kN·m/kg
Stiffness to weight25.3MN·m/kg12.6x higher2.01MN·m/kg
Poisson's ratio0.333base material0.384
Shear modulus25.7GPa29.6x stiffer in shear0.867GPa
Bulk modulus67GPa20.1x higher3.33GPa
Speed of sound5,030m/s3.55x faster1,418m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6FDM Polycarbonate
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6FDM Polycarbonate
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 6061-T6FDM Polycarbonate
Thermal conductivity167W/m·K1835x more heat through a finbase material0.2W/m·K5
Thermal expansion23.6µm/m·K12.75x lessbase material65µm/m·K5
100 mm part over a 50 °C swing118µm growth2.75x less325µm growth
Specific heat896J/kg·K1not sourced
Heats up and cools (diffusivity)69mm²/snot sourced
Thermal shock resistance19,159W/m451x more resistant42.5W/m
Melting pointsolidus-liquidus582–652°C1not sourced
Glass transitionnot sourced108°C2
Max service temperaturenot sourcedHDT 0.455 MPa105°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6FDM Polycarbonate
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6FDM Polycarbonate
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Kaiser Aluminum, UltiMaker, U.S. Department of Defense, Covestro
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
FDM Polycarbonate
Ultimaker PC, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 20, 2022.
  1. 1
    Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
  2. 2
    Ultimaker PC Technical Data Sheet, v5.00UltiMakerarchived copyFDM Polycarbonate · Yield strength: typicalFDM Polycarbonate · Ultimate tensile strength: typical, peak stress (= stress at yield)FDM Polycarbonate · Flexural strength: typicalFDM Polycarbonate · Elongation at break: typicalFDM Polycarbonate · Young's modulus (stiffness): typicalFDM Polycarbonate · Density: rangeFDM Polycarbonate · Glass transition: typicalFDM Polycarbonate · Max service temperature: HDT 0.455 MPa (printed specimens)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)
  4. 4
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyFDM Polycarbonate · Poisson's ratio: base material: polycarbonate family typical (Covestro Part and Mold Design guide, Table 3-1)
  5. 5
    Makrolon 2405 Technical Data SheetCovestroFDM Polycarbonate · Thermal conductivity: base material: Covestro Makrolon 2405 injection-molding PC, typical, through-plane, 23 °CFDM Polycarbonate · Thermal expansion: base material: Covestro Makrolon 2405 injection-molding PC, typical, 23-55 °C, parallel

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM Polycarbonate is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 6061-T6 stronger than FDM Polycarbonate?

Aluminum 6061-T6 is stronger: its yield strength is 276 MPa against 53.3 MPa for FDM Polycarbonate (5.18x).

Which is lighter, Aluminum 6061-T6 or FDM Polycarbonate?

FDM Polycarbonate is lighter: 1,190 kg/m³ against 2,700 kg/m³ for Aluminum 6061-T6.

Which is stiffer, Aluminum 6061-T6 or FDM Polycarbonate?

Aluminum 6061-T6 is stiffer: Young's modulus 68.3 GPa against 2.39 GPa for FDM Polycarbonate, so the same part in Aluminum 6061-T6 deflects less under the same load.

Which is lighter for the same job, Aluminum 6061-T6 or FDM Polycarbonate?

For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam.

Part that must beAluminum 6061-T6FDM Polycarbonate
Stiff rod or tie (tension)lighter12.6x heavier
Stiff beam (bending)lighter2.35x heavier
Stiff panel or platelighter35% heavier
Strong rod or tielighter2.28x heavier
Strong beamlighter32% heavier
Strong panel or plateabout equalabout equal

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 6061-T6 or FDM Polycarbonate?

Aluminum 6061-T6 stretches further before it breaks: 17% elongation at break against 9.2% for FDM Polycarbonate.

Thermal

Which conducts heat better, Aluminum 6061-T6 or FDM Polycarbonate?

Aluminum 6061-T6 conducts heat better: 167 W/m·K against 0.2 W/m·K for FDM Polycarbonate.

Which expands less with temperature?

Aluminum 6061-T6 expands less: 23.6 µm/m·K against 65 µm/m·K for FDM Polycarbonate.

Related comparisons