Materials / Compare

Aluminum 7050-T7451 vs. Brass C260

Compare Aluminum 7050-T7451 vs. Brass C260 strength, stiffness, weight and thermal properties.

Aluminum 7050-T7451Wrought
Brass C260Wrought
MechanicalAluminum 7050-T7451Brass C260
Yield strength469MPa136% stronger345MPa2
Ultimate tensile strength524MPa123% stronger427MPa2
Elongation at break11%123%22.09x more ductile
Young's modulus (stiffness)70.3GPa1110GPa31.57x stiffer
Density2,830kg/m³13.01x lighter8,525kg/m³3
Strength to weight166kN·m/kg4.1x higher40.5kN·m/kg
Stiffness to weight24.8MN·m/kg1.92x higher12.9MN·m/kg
Poisson's ratio0.3340.345
Shear modulus26.4GPa41.2GPa1.56x stiffer in shear
Bulk modulus68.9GPa115GPa1.67x higher
Speed of sound4,984m/s39% faster3,597m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Brass C260
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Brass C260
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7050-T7451Brass C260
Thermal conductivity157W/m·K130% more heat through a fin121W/m·K3
Thermal expansion23.5µm/m·K120µm/m·K318% less
100 mm part over a 50 °C swing118µm growth100µm growth18% less
Specific heat860J/kg·K12.28x higher377J/kg·K3
Heats up and cools (diffusivity)64.5mm²/s1.71x faster37.7mm²/s
Thermal shock resistance29,862W/m2.39x more resistant12,510W/m
Melting pointmelting range524–635°C1solidus-liquidus916–954°C3
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Brass C260
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Brass C260
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Kaiser Aluminum, Copper Development Association, U.S. Department of Defense, Wieland
Aluminum 7050-T7451
7050-T7451 plate, Kaiser Aluminum sheet, coil & plate typical datasheet (longitudinal); Poisson from MIL-HDBK-5J
Brass C260
C26000 cartridge brass, H02 half hard flat/strip: CDA Electronic Connector Design Guide (mechanical) + CDA alloy page (physical)
  1. 1
    Alloy 7050 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7050-T7451 · Yield strength: typical, longitudinal, 0.2% offsetAluminum 7050-T7451 · Ultimate tensile strength: typical, longitudinalAluminum 7050-T7451 · Elongation at break: typical, longitudinalAluminum 7050-T7451 · Young's modulus (stiffness): typicalAluminum 7050-T7451 · Density: nominalAluminum 7050-T7451 · Thermal conductivity: typical, 20 °CAluminum 7050-T7451 · Thermal expansion: typical, mean 20-100 °CAluminum 7050-T7451 · Specific heat: typical, at 100 °CAluminum 7050-T7451 · Melting point: melting range
  2. 2
    Electronic Connector Design Guide: Cold Rolled TempersCopper Development Associationarchived copyBrass C260 · Yield strength: nominal, strip/flat, 0.5% extension (not 0.2% offset)Brass C260 · Ultimate tensile strength: nominal, strip/flatBrass C260 · Elongation at break: nominal, in 2.0 in., strip/flat
  3. 3
    C26000 Alloy (copper.org)Copper Development Associationarchived copyBrass C260 · Young's modulus (stiffness): typical, temper-independentBrass C260 · Density: nominalBrass C260 · Thermal conductivity: typical, 20 °CBrass C260 · Thermal expansion: typical, mean 20-300 °CBrass C260 · Specific heat: typical, 20 °CBrass C260 · Melting point: solidus-liquidus
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7050-T7451 · Poisson's ratio: typical (handbook physical constant)
  5. 5
    Wieland-M30 (CuZn30, C26000) Data SheetWielandarchived copyBrass C260 · Poisson's ratio: reference value at room temperature (Wieland-M30 = CuZn30 = C26000, rolled products)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 7050-T7451 stronger than Brass C260?

Aluminum 7050-T7451 is stronger: its yield strength is 469 MPa against 345 MPa for Brass C260 (36%).

Which is lighter, Aluminum 7050-T7451 or Brass C260?

Aluminum 7050-T7451 is lighter: 2,830 kg/m³ against 8,525 kg/m³ for Brass C260.

Which is stiffer, Aluminum 7050-T7451 or Brass C260?

Brass C260 is stiffer: Young's modulus 110 GPa against 70.3 GPa for Aluminum 7050-T7451, so the same part in Brass C260 deflects less under the same load.

Which is lighter for the same job, Aluminum 7050-T7451 or Brass C260?

For the same stiffness or strength: Aluminum 7050-T7451 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7050-T7451Brass C260
Stiff rod or tie (tension)lighter1.92x heavier
Stiff beam (bending)lighter2.4x heavier
Stiff panel or platelighter2.59x heavier
Strong rod or tielighter4.1x heavier
Strong beamlighter3.7x heavier
Strong panel or platelighter3.51x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7050-T7451 or Brass C260?

Brass C260 stretches further before it breaks: 23% elongation at break against 11% for Aluminum 7050-T7451.

Thermal

Which conducts heat better, Aluminum 7050-T7451 or Brass C260?

Aluminum 7050-T7451 conducts heat better: 157 W/m·K against 121 W/m·K for Brass C260.

Which expands less with temperature?

Brass C260 expands less: 20 µm/m·K against 23.5 µm/m·K for Aluminum 7050-T7451.

Related comparisons