Materials / Compare

Aluminum 7050-T7451 vs. FDM PAHT-CF

Compare Aluminum 7050-T7451 vs. FDM PAHT-CF strength, stiffness, weight and thermal properties.

Aluminum 7050-T7451Wrought
FDM PAHT-CF3D printed (FDM)
MechanicalAluminum 7050-T7451FDM PAHT-CF
Yield strength469MPa1not given (tensile used)
Ultimate tensile strength524MPa15.7x stronger92MPa2
Flexural strengthnot sourced125MPa2
Elongation at break11%131% more ductile8.4%2
Young's modulus (stiffness)70.3GPa118.2x stiffer3.86GPa2
Density2,830kg/m³11,060kg/m³22.67x lighter
Strength to weight166kN·m/kg1.91x higher86.8kN·m/kg
Stiffness to weight24.8MN·m/kg6.82x higher3.64MN·m/kg
Poisson's ratio0.333not sourced
Shear modulus26.4GPanot sourced
Bulk modulus68.9GPanot sourced
Speed of sound4,984m/s2.61x faster1,908m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451FDM PAHT-CF
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451FDM PAHT-CF
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7050-T7451FDM PAHT-CF
Thermal conductivity157W/m·K1not sourced
Thermal expansion23.5µm/m·K1not sourced
100 mm part over a 50 °C swing118µm growthnot sourced
Specific heat860J/kg·K1not sourced
Heats up and cools (diffusivity)64.5mm²/snot sourced
Thermal shock resistance29,862W/mnot sourced
Melting pointmelting range524–635°C1225°C2
Glass transitionnot sourced70°C2
Max service temperaturenot sourcedHDT 1.8 MPa170°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: Kaiser Aluminum, Bambu Lab, U.S. Department of Defense
Aluminum 7050-T7451
7050-T7451 plate, Kaiser Aluminum sheet, coil & plate typical datasheet (longitudinal); Poisson from MIL-HDBK-5J
FDM PAHT-CF
Bambu Lab PAHT-CF, TDS V3.0, printed specimens X-Y, dry state; nozzle 290 °C, bed 100 °C, 100 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
  1. 1
    Alloy 7050 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7050-T7451 · Yield strength: typical, longitudinal, 0.2% offsetAluminum 7050-T7451 · Ultimate tensile strength: typical, longitudinalAluminum 7050-T7451 · Elongation at break: typical, longitudinalAluminum 7050-T7451 · Young's modulus (stiffness): typicalAluminum 7050-T7451 · Density: nominalAluminum 7050-T7451 · Thermal conductivity: typical, 20 °CAluminum 7050-T7451 · Thermal expansion: typical, mean 20-100 °CAluminum 7050-T7451 · Specific heat: typical, at 100 °CAluminum 7050-T7451 · Melting point: melting range
  2. 2
    Bambu PAHT-CF Technical Data Sheet, V3.0Bambu LabFDM PAHT-CF · Ultimate tensile strength: typicalFDM PAHT-CF · Flexural strength: typicalFDM PAHT-CF · Elongation at break: typicalFDM PAHT-CF · Young's modulus (stiffness): typicalFDM PAHT-CF · Density: typicalFDM PAHT-CF · Melting point: typicalFDM PAHT-CF · Glass transition: typicalFDM PAHT-CF · Max service temperature: HDT 1.8 MPa
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7050-T7451 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM PAHT-CF is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 7050-T7451 stronger than FDM PAHT-CF?

Aluminum 7050-T7451 is stronger: its yield strength is 469 MPa against tensile strength 92 MPa for FDM PAHT-CF (5.1x).

Which is lighter, Aluminum 7050-T7451 or FDM PAHT-CF?

FDM PAHT-CF is lighter: 1,060 kg/m³ against 2,830 kg/m³ for Aluminum 7050-T7451.

Which is stiffer, Aluminum 7050-T7451 or FDM PAHT-CF?

Aluminum 7050-T7451 is stiffer: Young's modulus 70.3 GPa against 3.86 GPa for FDM PAHT-CF, so the same part in Aluminum 7050-T7451 deflects less under the same load.

Which is lighter for the same job, Aluminum 7050-T7451 or FDM PAHT-CF?

For the same stiffness or strength: Aluminum 7050-T7451 is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam; FDM PAHT-CF is lighter for a stiff panel or plate, strong panel or plate.

Part that must beAluminum 7050-T7451FDM PAHT-CF
Stiff rod or tie (tension)lighter6.82x heavier
Stiff beam (bending)lighter1.6x heavier
Stiff panel or plate1% heavierlighter
Strong rod or tielighter1.91x heavier
Strong beamlighter11% heavier
Strong panel or plate18% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7050-T7451 or FDM PAHT-CF?

Aluminum 7050-T7451 stretches further before it breaks: 11% elongation at break against 8.4% for FDM PAHT-CF.