Materials / Compare

DMLS AlSi10Mg Aluminum vs. Plastic HDPE

Compare DMLS AlSi10Mg Aluminum vs. Plastic HDPE strength, stiffness, weight and thermal properties.

DMLS AlSi10Mg Aluminum3D printed metal (DMLS)
Plastic HDPEBulk polymer (molded or machined)
MechanicalDMLS AlSi10Mg AluminumPlastic HDPE
Yield strength270MPa111.3x stronger24MPa2
Ultimate tensile strength450MPa1not stated (yield given)
Elongation at break10.2%1not sourced
Young's modulus (stiffness)72GPa380x stiffer0.9GPa2
Density2,670kg/m³4950kg/m³22.81x lighter
Strength to weight101kN·m/kg4x higher25.3kN·m/kg
Stiffness to weight27MN·m/kg28.5x higher0.947MN·m/kg
Poisson's ratiobase material0.335base material0.4–0.456
Shear modulus27.1GPa85.7x stiffer in shear0.316GPa
Bulk modulus70.6GPa35.3x higher2GPa
Speed of sound5,193m/s5.34x faster973m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic HDPE
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic HDPE
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS AlSi10Mg AluminumPlastic HDPE
Thermal conductivity110W/m·K1base material0.4–0.49W/m·K6
Thermal expansionmean 25-100 °C20µm/m·K16x lessbase material120µm/m·K6
100 mm part over a 50 °C swing100µm growth6x less600µm growth
Specific heatbase material963J/kg·K5base material2,250J/kg·K6
Heats up and cools (diffusivity)42.8mm²/s205x faster0.208mm²/s
Thermal shock resistance13,819W/m243x more resistant56.9W/m
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic HDPE
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic HDPE
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: EOS GmbH, LyondellBasell, Renishaw, U.S. Department of Defense, INEOS Olefins & Polymers USA
DMLS AlSi10Mg Aluminum
EOS Aluminium AlSi10Mg (powder 9011-0024), EOS M 290 | 30 µm process (AlSi10Mg_FlexM291 2.01), as manufactured, horizontal; machined (turned) specimens, ISO 6892-1 B10
Plastic HDPE
LyondellBasell Hostalen 23050 B high density polyethylene, typical ISO values
  1. 1
    EOS Aluminium AlSi10Mg Material Data SheetEOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Yield strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Ultimate tensile strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Elongation at break: typical at break, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Thermal conductivity: typical, as manufactured, horizontal (ISO 22007-2)DMLS AlSi10Mg Aluminum · Thermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    Hostalen 23050 B Product DataLyondellBasellPlastic HDPE · Yield strength: typical, tensile stress at yield 23 °C, 50 mm/min ISO 527Plastic HDPE · Young's modulus (stiffness): typical, tensile modulus 23 °C ISO 527Plastic HDPE · Density: typical, ISO 1183
  3. 3
    RenAM 500 Series Aluminium AlSi10Mg Material Data SheetRenishawDMLS AlSi10Mg Aluminum · Young's modulus (stiffness): same material and process, different machine maker: Renishaw RenAM 500, 30 µm, as built, horizontal (XY)
  4. 4
    EOS Aluminium AlSi10Mg Material Data Sheet, FlexLine, M 290 (2018)EOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Density: typical part density (ISO 3369), EOS M 290, AlSi10Mg_030_FlexM291 (30 µm)
  5. 5
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseDMLS AlSi10Mg Aluminum · Poisson's ratio: base material: cast Al-Si-Mg alloy 359.0 (Al-9Si-0.6Mg, closest MIL-HDBK-5J alloy to AlSi10Mg / EN AC-43000)DMLS AlSi10Mg Aluminum · Specific heat: base material: cast Al-Si-Mg alloy 359.0 (MIL-HDBK-5J), at 100 °C
  6. 6
    Typical Engineering Properties of High Density PolyethyleneINEOS Olefins & Polymers USAarchived copyPlastic HDPE · Poisson's ratio: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Thermal conductivity: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Thermal expansion: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Specific heat: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS AlSi10Mg Aluminum is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS AlSi10Mg Aluminum stronger than Plastic HDPE?

DMLS AlSi10Mg Aluminum is stronger: its yield strength is 270 MPa against 24 MPa for Plastic HDPE (11.3x).

Which is lighter, DMLS AlSi10Mg Aluminum or Plastic HDPE?

Plastic HDPE is lighter: 950 kg/m³ against 2,670 kg/m³ for DMLS AlSi10Mg Aluminum.

Which is stiffer, DMLS AlSi10Mg Aluminum or Plastic HDPE?

DMLS AlSi10Mg Aluminum is stiffer: Young's modulus 72 GPa against 0.9 GPa for Plastic HDPE, so the same part in DMLS AlSi10Mg Aluminum deflects less under the same load.

Which is lighter for the same job, DMLS AlSi10Mg Aluminum or Plastic HDPE?

For the same stiffness or strength: DMLS AlSi10Mg Aluminum is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beDMLS AlSi10Mg AluminumPlastic HDPE
Stiff rod or tie (tension)lighter28.5x heavier
Stiff beam (bending)lighter3.18x heavier
Stiff panel or platelighter1.53x heavier
Strong rod or tielighter4x heavier
Strong beamlighter1.79x heavier
Strong panel or platelighter19% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, DMLS AlSi10Mg Aluminum or Plastic HDPE?

DMLS AlSi10Mg Aluminum conducts heat better: 110 W/m·K against 0.445 W/m·K for Plastic HDPE.

Which expands less with temperature?

DMLS AlSi10Mg Aluminum expands less: 20 µm/m·K against 120 µm/m·K for Plastic HDPE.

Related comparisons