Materials / Compare

DMLS AlSi10Mg Aluminum vs. Plastic UHMWPE

Compare DMLS AlSi10Mg Aluminum vs. Plastic UHMWPE strength, stiffness, weight and thermal properties.

DMLS AlSi10Mg Aluminum3D printed metal (DMLS)
Plastic UHMWPEBulk polymer (molded or machined)
MechanicalDMLS AlSi10Mg AluminumPlastic UHMWPE
Yield strength270MPa113.5x stronger20MPa2
Ultimate tensile strength450MPa143MPa2
Elongation at break10.2%1465%245.6x more ductile
Young's modulus (stiffness)72GPa3109x stiffer0.66GPa2
Density2,670kg/m³4930kg/m³22.87x lighter
Strength to weight101kN·m/kg4.7x higher21.5kN·m/kg
Stiffness to weight27MN·m/kg38x higher0.71MN·m/kg
Poisson's ratiobase material0.335not sourced
Shear modulus27.1GPanot sourced
Bulk modulus70.6GPanot sourced
Speed of sound5,193m/s6.16x faster842m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic UHMWPE
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic UHMWPE
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS AlSi10Mg AluminumPlastic UHMWPE
Thermal conductivity110W/m·K1275x more heat through a fin0.4W/m·K6
Thermal expansionmean 25-100 °C20µm/m·K110x less200µm/m·K6
100 mm part over a 50 °C swing100µm growth10x less1,000µm growth
Specific heatbase material963J/kg·K5not sourced
Heats up and cools (diffusivity)42.8mm²/snot sourced
Thermal shock resistance13,819W/mnot sourced
Melting pointnot sourcedDSC 10 K/min130–138°C2
Max service temperaturenot sourced80°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic UHMWPE
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumPlastic UHMWPE
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: EOS GmbH, Celanese, Renishaw, U.S. Department of Defense
DMLS AlSi10Mg Aluminum
EOS Aluminium AlSi10Mg (powder 9011-0024), EOS M 290 | 30 µm process (AlSi10Mg_FlexM291 2.01), as manufactured, horizontal; machined (turned) specimens, ISO 6892-1 B10
Plastic UHMWPE
Celanese GUR 4120 (avg. molecular weight 4.7x10^6 g/mol), typical values on compression-molded specimens; CTE and thermal conductivity from Celanese's generic UHMWPE guide (grade not named)
  1. 1
    EOS Aluminium AlSi10Mg Material Data SheetEOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Yield strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Ultimate tensile strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Elongation at break: typical at break, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Thermal conductivity: typical, as manufactured, horizontal (ISO 22007-2)DMLS AlSi10Mg Aluminum · Thermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    GUR UHMW-PE Overview (GUR-015)CelanesePlastic UHMWPE · Yield strength: typical, tensile stress at yield ISO 527, 50 mm/minPlastic UHMWPE · Ultimate tensile strength: typical, tensile stress at break ISO 527, 50 mm/minPlastic UHMWPE · Elongation at break: typical, nominal elongation at break ISO 527Plastic UHMWPE · Young's modulus (stiffness): typical, tensile modulus ISO 527, 1 mm/minPlastic UHMWPE · Density: typicalPlastic UHMWPE · Melting point: DSC 10 K/minPlastic UHMWPE · Max service temperature: recommended max constant operating temperature
  3. 3
    RenAM 500 Series Aluminium AlSi10Mg Material Data SheetRenishawDMLS AlSi10Mg Aluminum · Young's modulus (stiffness): same material and process, different machine maker: Renishaw RenAM 500, 30 µm, as built, horizontal (XY)
  4. 4
    EOS Aluminium AlSi10Mg Material Data Sheet, FlexLine, M 290 (2018)EOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Density: typical part density (ISO 3369), EOS M 290, AlSi10Mg_030_FlexM291 (30 µm)
  5. 5
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseDMLS AlSi10Mg Aluminum · Poisson's ratio: base material: cast Al-Si-Mg alloy 359.0 (Al-9Si-0.6Mg, closest MIL-HDBK-5J alloy to AlSi10Mg / EN AC-43000)DMLS AlSi10Mg Aluminum · Specific heat: base material: cast Al-Si-Mg alloy 359.0 (MIL-HDBK-5J), at 100 °C
  6. 6
    GUR UHMW-PE Polymer Guide (GUR-003)Celanesearchived copyPlastic UHMWPE · Thermal conductivity: typical, unfilled (narrative value, generic Celanese UHMWPE)Plastic UHMWPE · Thermal expansion: typical, 20 to 100 °C (generic Celanese UHMWPE)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS AlSi10Mg Aluminum is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS AlSi10Mg Aluminum stronger than Plastic UHMWPE?

DMLS AlSi10Mg Aluminum is stronger: its yield strength is 270 MPa against 20 MPa for Plastic UHMWPE (13.5x).

Which is lighter, DMLS AlSi10Mg Aluminum or Plastic UHMWPE?

Plastic UHMWPE is lighter: 930 kg/m³ against 2,670 kg/m³ for DMLS AlSi10Mg Aluminum.

Which is stiffer, DMLS AlSi10Mg Aluminum or Plastic UHMWPE?

DMLS AlSi10Mg Aluminum is stiffer: Young's modulus 72 GPa against 0.66 GPa for Plastic UHMWPE, so the same part in DMLS AlSi10Mg Aluminum deflects less under the same load.

Which is lighter for the same job, DMLS AlSi10Mg Aluminum or Plastic UHMWPE?

For the same stiffness or strength: DMLS AlSi10Mg Aluminum is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beDMLS AlSi10Mg AluminumPlastic UHMWPE
Stiff rod or tie (tension)lighter38x heavier
Stiff beam (bending)lighter3.64x heavier
Stiff panel or platelighter1.66x heavier
Strong rod or tielighter4.7x heavier
Strong beamlighter1.97x heavier
Strong panel or platelighter28% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, DMLS AlSi10Mg Aluminum or Plastic UHMWPE?

Plastic UHMWPE stretches further before it breaks: 465% elongation at break against 10.2% for DMLS AlSi10Mg Aluminum.

Thermal

Which conducts heat better, DMLS AlSi10Mg Aluminum or Plastic UHMWPE?

DMLS AlSi10Mg Aluminum conducts heat better: 110 W/m·K against 0.4 W/m·K for Plastic UHMWPE.

Which expands less with temperature?

DMLS AlSi10Mg Aluminum expands less: 20 µm/m·K against 200 µm/m·K for Plastic UHMWPE.

Related comparisons