MechanicalDMLS AlSi10Mg AluminumStainless Steel 17-4PH
Yield strength270MPa11,275MPa24.72x stronger
Ultimate tensile strength450MPa11,379MPa23.06x stronger
Elongation at break10.2%113% more ductile9%2
Young's modulus (stiffness)72GPa3H 900197GPa22.74x stiffer
Density2,670kg/m³42.92x lighterH 9007,800kg/m³2
Strength to weight101kN·m/kg163kN·m/kg1.62x higher
Stiffness to weight27MN·m/kg7% higher25.3MN·m/kg
Poisson's ratiobase material0.335H 9000.2722
Shear modulus27.1GPa77.4GPa2.86x stiffer in shear
Bulk modulus70.6GPa144GPa2.04x higher
Speed of sound5,193m/s3% faster5,026m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumStainless Steel 17-4PH
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumStainless Steel 17-4PH
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS AlSi10Mg AluminumStainless Steel 17-4PH
Thermal conductivity110W/m·K16.15x more heat through a finat 149 °C17.9W/m·K2
Thermal expansionmean 25-100 °C20µm/m·K1mean10.8µm/m·K21.85x less
100 mm part over a 50 °C swing100µm growth54µm growth1.85x less
Specific heatbase material963J/kg·K5mean460J/kg·K2
Heats up and cools (diffusivity)42.8mm²/s8.58x faster4.99mm²/s
Thermal shock resistance13,819W/m1.77x more resistant7,809W/m
Max service temperaturenot sourced316°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumStainless Steel 17-4PH
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumStainless Steel 17-4PH
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: EOS GmbH, Cleveland-Cliffs, Renishaw, U.S. Department of Defense
DMLS AlSi10Mg Aluminum
EOS Aluminium AlSi10Mg (powder 9011-0024), EOS M 290 | 30 µm process (AlSi10Mg_FlexM291 2.01), as manufactured, horizontal; machined (turned) specimens, ISO 6892-1 B10
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
  1. 1
    EOS Aluminium AlSi10Mg Material Data SheetEOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Yield strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Ultimate tensile strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Elongation at break: typical at break, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Thermal conductivity: typical, as manufactured, horizontal (ISO 22007-2)DMLS AlSi10Mg Aluminum · Thermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
  3. 3
    RenAM 500 Series Aluminium AlSi10Mg Material Data SheetRenishawDMLS AlSi10Mg Aluminum · Young's modulus (stiffness): same material and process, different machine maker: Renishaw RenAM 500, 30 µm, as built, horizontal (XY)
  4. 4
    EOS Aluminium AlSi10Mg Material Data Sheet, FlexLine, M 290 (2018)EOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Density: typical part density (ISO 3369), EOS M 290, AlSi10Mg_030_FlexM291 (30 µm)
  5. 5
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseDMLS AlSi10Mg Aluminum · Poisson's ratio: base material: cast Al-Si-Mg alloy 359.0 (Al-9Si-0.6Mg, closest MIL-HDBK-5J alloy to AlSi10Mg / EN AC-43000)DMLS AlSi10Mg Aluminum · Specific heat: base material: cast Al-Si-Mg alloy 359.0 (MIL-HDBK-5J), at 100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS AlSi10Mg Aluminum is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS AlSi10Mg Aluminum stronger than Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 270 MPa for DMLS AlSi10Mg Aluminum (4.72x).

Which is lighter, DMLS AlSi10Mg Aluminum or Stainless Steel 17-4PH?

DMLS AlSi10Mg Aluminum is lighter: 2,670 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.

Which is stiffer, DMLS AlSi10Mg Aluminum or Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 72 GPa for DMLS AlSi10Mg Aluminum, so the same part in Stainless Steel 17-4PH deflects less under the same load.

Which is lighter for the same job, DMLS AlSi10Mg Aluminum or Stainless Steel 17-4PH?

For the same stiffness or strength: DMLS AlSi10Mg Aluminum is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; Stainless Steel 17-4PH is lighter for a strong rod or tie.

Part that must beDMLS AlSi10Mg AluminumStainless Steel 17-4PH
Stiff rod or tie (tension)lighter7% heavier
Stiff beam (bending)lighter1.77x heavier
Stiff panel or platelighter2.09x heavier
Strong rod or tie1.62x heavierlighter
Strong beamlighter4% heavier
Strong panel or platelighter34% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, DMLS AlSi10Mg Aluminum or Stainless Steel 17-4PH?

DMLS AlSi10Mg Aluminum stretches further before it breaks: 10.2% elongation at break against 9% for Stainless Steel 17-4PH.

Thermal

Which conducts heat better, DMLS AlSi10Mg Aluminum or Stainless Steel 17-4PH?

DMLS AlSi10Mg Aluminum conducts heat better: 110 W/m·K against 17.9 W/m·K for Stainless Steel 17-4PH.

Which expands less with temperature?

Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 20 µm/m·K for DMLS AlSi10Mg Aluminum.

Related comparisons