Materials / Compare

Plastic PETG vs. Steel AISI 1045

Compare Plastic PETG vs. Steel AISI 1045 strength, stiffness, weight and thermal properties.

Plastic PETG3D printed (FDM)
Steel AISI 1045Wrought
MechanicalPlastic PETGSteel AISI 1045
Yield strength46.2MPa1producer-stated531MPa211.5x stronger
Ultimate tensile strength46.2MPa1producer-stated627MPa213.6x stronger
Flexural strength78.9MPa1not sourced
Elongation at break7.6%1in 2 in12%21.58x more ductile
Young's modulus (stiffness)1.94GPa1210GPa3108x stiffer
Density1,270kg/m³16.14x lighter7,800kg/m³3
Strength to weight36.4kN·m/kg68.1kN·m/kg1.87x higher
Stiffness to weight1.53MN·m/kg26.9MN·m/kg17.6x higher
Poisson's rationot sourced0.33
Shear modulusnot sourced80.8GPa
Bulk modulusnot sourced175GPa
Speed of sound1,236m/s5,189m/s4.2x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PETGSteel AISI 1045
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PETGSteel AISI 1045
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic PETGSteel AISI 1045
Thermal conductivitybase material0.21W/m·K440–45W/m·K3
Thermal expansionbase material51µm/m·K412µm/m·K34.25x less
100 mm part over a 50 °C swing255µm growth60µm growth4.25x less
Specific heatbase material1,300J/kg·K4460–480J/kg·K3
Heats up and cools (diffusivity)0.127mm²/s11.6mm²/s91.1x faster
Thermal shock resistancenot sourced6,269W/m
Glass transition77.4°C1not sourced
Max service temperatureHDT 0.455 MPa76.2°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PETGSteel AISI 1045
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PETGSteel AISI 1045
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: UltiMaker, Niagara LaSalle, Ovako, Eastman
Plastic PETG
Ultimaker PETG, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v1.00, April 29, 2022.
Steel AISI 1045
AISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants
  1. 1
    Ultimaker PETG Technical Data Sheet, v1.00UltiMakerarchived copyPlastic PETG · Yield strength: typicalPlastic PETG · Ultimate tensile strength: typical, peak stress (= stress at yield)Plastic PETG · Flexural strength: typicalPlastic PETG · Elongation at break: typicalPlastic PETG · Young's modulus (stiffness): typicalPlastic PETG · Density: typicalPlastic PETG · Glass transition: typicalPlastic PETG · Max service temperature: HDT 0.455 MPa (printed specimens)
  2. 2
    1045 PropertiesNiagara LaSallearchived copySteel AISI 1045 · Yield strength: producer-stated, cold drawnSteel AISI 1045 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1045 · Elongation at break: in 2 in (50.8 mm)
  3. 3
    C45 Steel GradeOvakoSteel AISI 1045 · Young's modulus (stiffness): typicalSteel AISI 1045 · Density: typicalSteel AISI 1045 · Poisson's ratio: typicalSteel AISI 1045 · Thermal conductivity: typical range, ambientSteel AISI 1045 · Thermal expansion: typical, mean 20-300 °CSteel AISI 1045 · Specific heat: typical range, 50/100 °C
  4. 4
    Eastar Copolyester 6763 Product Data SheetEastmanPlastic PETG · Thermal conductivity: base material: Eastman Eastar Copolyester 6763 (PETG), typicalPlastic PETG · Thermal expansion: base material: Eastman Eastar Copolyester 6763 (PETG), typicalPlastic PETG · Specific heat: base material: Eastman Eastar Copolyester 6763 (PETG), DSC at 60 °C (lowest temperature listed)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic PETG is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Plastic PETG stronger than Steel AISI 1045?

Steel AISI 1045 is stronger: its yield strength is 531 MPa against 46.2 MPa for Plastic PETG (11.5x).

Which is lighter, Plastic PETG or Steel AISI 1045?

Plastic PETG is lighter: 1,270 kg/m³ against 7,800 kg/m³ for Steel AISI 1045.

Which is stiffer, Plastic PETG or Steel AISI 1045?

Steel AISI 1045 is stiffer: Young's modulus 210 GPa against 1.94 GPa for Plastic PETG, so the same part in Steel AISI 1045 deflects less under the same load.

Which is lighter for the same job, Plastic PETG or Steel AISI 1045?

For the same stiffness or strength: Plastic PETG is lighter for a stiff panel or plate, strong beam, strong panel or plate; Steel AISI 1045 is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie.

Part that must bePlastic PETGSteel AISI 1045
Stiff rod or tie (tension)17.6x heavierlighter
Stiff beam (bending)1.69x heavierlighter
Stiff panel or platelighter29% heavier
Strong rod or tie1.87x heavierlighter
Strong beamlighter21% heavier
Strong panel or platelighter1.81x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic PETG or Steel AISI 1045?

Steel AISI 1045 stretches further before it breaks: 12% elongation at break against 7.6% for Plastic PETG.

Thermal

Which conducts heat better, Plastic PETG or Steel AISI 1045?

Steel AISI 1045 conducts heat better: 42.5 W/m·K against 0.21 W/m·K for Plastic PETG.

Which expands less with temperature?

Steel AISI 1045 expands less: 12 µm/m·K against 51 µm/m·K for Plastic PETG.

Related comparisons