Aluminum 7050-T7451 vs. DMLS 17-4PH Stainless Steel
Compare Aluminum 7050-T7451 vs. DMLS 17-4PH Stainless Steel strength, stiffness, weight and thermal properties.
| Mechanical | Aluminum 7050-T7451 | DMLS 17-4PH Stainless Steel |
|---|---|---|
| Yield strength | 469MPa1 | mean861MPa21.83x stronger |
| Ultimate tensile strength | 524MPa1 | mean886MPa21.69x stronger |
| Elongation at break | 11%1 | mean at break19.9%21.81x more ductile |
| Young's modulus (stiffness) | 70.3GPa1 | base material197GPa32.8x stiffer |
| Density | 2,830kg/m³12.75x lighter | mean part density7,790kg/m³2 |
| Strength to weight | 166kN·m/kg1.5x higher | 110kN·m/kg |
| Stiffness to weight | 24.8MN·m/kg | 25.3MN·m/kg2% higher |
| Poisson's ratio | 0.334 | base material0.2723 |
| Shear modulus | 26.4GPa | 77.4GPa2.93x stiffer in shear |
| Bulk modulus | 68.9GPa | 144GPa2.09x higher |
| Speed of sound | 4,984m/s | 5,029m/s |
| Thermal | Aluminum 7050-T7451 | DMLS 17-4PH Stainless Steel |
|---|---|---|
| Thermal conductivity | 157W/m·K18.77x more heat through a fin | base material17.9W/m·K3 |
| Thermal expansion | 23.5µm/m·K1 | mean 25-100 °C10.4µm/m·K22.26x less |
| 100 mm part over a 50 °C swing | 118µm growth | 52µm growth2.26x less |
| Specific heat | 860J/kg·K11.87x higher | base material460J/kg·K3 |
| Heats up and cools (diffusivity) | 64.5mm²/s12.9x faster | 5mm²/s |
| Thermal shock resistance | 29,862W/m5.46x more resistant | 5,474W/m |
| Melting point | melting range524–635°C1 | not sourced |
| Try it on a partA bracket to run stress or thermal on, free in your browser | Open in LessCAD | Open in LessCAD |
|---|
Sources4 documents: Kaiser Aluminum, EOS GmbH, Cleveland-Cliffs, U.S. Department of Defense
- Aluminum 7050-T7451
- 7050-T7451 plate, Kaiser Aluminum sheet, coil & plate typical datasheet (longitudinal); Poisson from MIL-HDBK-5J
- DMLS 17-4PH Stainless Steel
- EOS StainlessSteel 17-4PH IndustryLine (powder 9011-0041), EOS M 290, 40 µm, default job 17-4PH_040_StainlessM291_100, as built, horizontal; ISO 6892 & ASTM E8M
- 1Alloy 7050 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7050-T7451 · Yield strength: typical, longitudinal, 0.2% offsetAluminum 7050-T7451 · Ultimate tensile strength: typical, longitudinalAluminum 7050-T7451 · Elongation at break: typical, longitudinalAluminum 7050-T7451 · Young's modulus (stiffness): typicalAluminum 7050-T7451 · Density: nominalAluminum 7050-T7451 · Thermal conductivity: typical, 20 °CAluminum 7050-T7451 · Thermal expansion: typical, mean 20-100 °CAluminum 7050-T7451 · Specific heat: typical, at 100 °CAluminum 7050-T7451 · Melting point: melting range
- 2EOS StainlessSteel 17-4PH IndustryLine Material Data Sheet, M 290EOS GmbHarchived copyDMLS 17-4PH Stainless Steel · Yield strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Ultimate tensile strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Elongation at break: mean at break, as built, horizontalDMLS 17-4PH Stainless Steel · Density: mean part density (ISO 3369)DMLS 17-4PH Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228, AFTER atmospheric heat treatment (as-built value not published)
- 317-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 17-4PH Stainless Steel · Young's modulus (stiffness): base material: wrought 17-4 PH, Condition H 900 (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Poisson's ratio: base material: wrought 17-4 PH, all conditions (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Thermal conductivity: base material: wrought 17-4 PH, Condition H 900, at 149 °C (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Specific heat: base material: wrought 17-4 PH, Condition A, 0-100 °C (Cleveland-Cliffs)
- 4MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7050-T7451 · Poisson's ratio: typical (handbook physical constant)
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
DMLS 17-4PH Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.
Questions
Mechanical
Is Aluminum 7050-T7451 stronger than DMLS 17-4PH Stainless Steel?
DMLS 17-4PH Stainless Steel is stronger: its yield strength is 861 MPa against 469 MPa for Aluminum 7050-T7451 (1.83x).
Which is lighter, Aluminum 7050-T7451 or DMLS 17-4PH Stainless Steel?
Aluminum 7050-T7451 is lighter: 2,830 kg/m³ against 7,790 kg/m³ for DMLS 17-4PH Stainless Steel.
Which is stiffer, Aluminum 7050-T7451 or DMLS 17-4PH Stainless Steel?
DMLS 17-4PH Stainless Steel is stiffer: Young's modulus 197 GPa against 70.3 GPa for Aluminum 7050-T7451, so the same part in DMLS 17-4PH Stainless Steel deflects less under the same load.
Which is lighter for the same job, Aluminum 7050-T7451 or DMLS 17-4PH Stainless Steel?
For the same stiffness or strength: Aluminum 7050-T7451 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; DMLS 17-4PH Stainless Steel is lighter for a stiff rod or tie (tension).
| Part that must be | Aluminum 7050-T7451 | DMLS 17-4PH Stainless Steel |
|---|---|---|
| Stiff rod or tie (tension) | 2% heavier | lighter |
| Stiff beam (bending) | lighter | 1.64x heavier |
| Stiff panel or plate | lighter | 1.95x heavier |
| Strong rod or tie | lighter | 1.5x heavier |
| Strong beam | lighter | 1.84x heavier |
| Strong panel or plate | lighter | 2.03x heavier |
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Aluminum 7050-T7451 or DMLS 17-4PH Stainless Steel?
DMLS 17-4PH Stainless Steel stretches further before it breaks: 19.9% elongation at break against 11% for Aluminum 7050-T7451.
Thermal
Which conducts heat better, Aluminum 7050-T7451 or DMLS 17-4PH Stainless Steel?
Aluminum 7050-T7451 conducts heat better: 157 W/m·K against 17.9 W/m·K for DMLS 17-4PH Stainless Steel.
Which expands less with temperature?
DMLS 17-4PH Stainless Steel expands less: 10.4 µm/m·K against 23.5 µm/m·K for Aluminum 7050-T7451.
Related comparisons
- Aluminum 7050-T7451 vs. Aluminum 7075-T6
- Aluminum 7050-T7451 vs. Aluminum 2024-T351
- Aluminum 7050-T7451 vs. Aluminum
- Aluminum 7050-T7451 vs. Aluminum 6061-T6
- DMLS 17-4PH Stainless Steel vs. Steel AISI 4340
- DMLS 17-4PH Stainless Steel vs. Nickel Inconel 718
- DMLS 17-4PH Stainless Steel vs. Stainless Steel 17-4PH
- DMLS 17-4PH Stainless Steel vs. Steel AISI 1045