Materials / Compare

Aluminum 7050-T7451 vs. DMLS 316L Stainless Steel

Compare Aluminum 7050-T7451 vs. DMLS 316L Stainless Steel strength, stiffness, weight and thermal properties.

Aluminum 7050-T7451Wrought
DMLS 316L Stainless Steel3D printed metal (DMLS)
MechanicalAluminum 7050-T7451DMLS 316L Stainless Steel
Yield strength469MPa1530MPa213% stronger
Ultimate tensile strength524MPa1640MPa222% stronger
Elongation at break11%140%23.64x more ductile
Young's modulus (stiffness)70.3GPa1185GPa32.63x stiffer
Density2,830kg/m³12.79x lighterpart density7,900kg/m³4
Strength to weight166kN·m/kg2.47x higher67.1kN·m/kg
Stiffness to weight24.8MN·m/kg6% higher23.4MN·m/kg
Poisson's ratio0.335base material0.36
Shear modulus26.4GPa71.2GPa2.69x stiffer in shear
Bulk modulus68.9GPa154GPa2.24x higher
Speed of sound4,984m/s3% faster4,839m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451DMLS 316L Stainless Steel
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451DMLS 316L Stainless Steel
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7050-T7451DMLS 316L Stainless Steel
Thermal conductivity157W/m·K19.69x more heat through a finbase material16.2W/m·K7
Thermal expansion23.5µm/m·K1mean 25-100 °C15.7µm/m·K249% less
100 mm part over a 50 °C swing118µm growth78.6µm growth49% less
Specific heat860J/kg·K11.72x higherbase material500J/kg·K7
Heats up and cools (diffusivity)64.5mm²/s15.7x faster4.1mm²/s
Thermal shock resistance29,862W/m14.4x more resistant2,067W/m
Melting pointmelting range524–635°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451DMLS 316L Stainless Steel
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451DMLS 316L Stainless Steel
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources7 documents: Kaiser Aluminum, EOS GmbH, U.S. Department of Defense, Steel Construction Institute, Cleveland-Cliffs
Aluminum 7050-T7451
7050-T7451 plate, Kaiser Aluminum sheet, coil & plate typical datasheet (longitudinal); Poisson from MIL-HDBK-5J
DMLS 316L Stainless Steel
EOS StainlessSteel 316L (powder 9011-0032), EOS M 290, ParameterSet 316L 20µm Surface M290/400W, as manufactured, horizontal; ISO 6892-1
  1. 1
    Alloy 7050 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7050-T7451 · Yield strength: typical, longitudinal, 0.2% offsetAluminum 7050-T7451 · Ultimate tensile strength: typical, longitudinalAluminum 7050-T7451 · Elongation at break: typical, longitudinalAluminum 7050-T7451 · Young's modulus (stiffness): typicalAluminum 7050-T7451 · Density: nominalAluminum 7050-T7451 · Thermal conductivity: typical, 20 °CAluminum 7050-T7451 · Thermal expansion: typical, mean 20-100 °CAluminum 7050-T7451 · Specific heat: typical, at 100 °CAluminum 7050-T7451 · Melting point: melting range
  2. 2
    EOS StainlessSteel 316L Material Data SheetEOS GmbHarchived copyDMLS 316L Stainless Steel · Yield strength: typical, as manufactured, horizontalDMLS 316L Stainless Steel · Ultimate tensile strength: typical, as manufactured, horizontalDMLS 316L Stainless Steel · Elongation at break: typical at break, as manufactured, horizontalDMLS 316L Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228
  3. 3
    EOS StainlessSteel 316L Material Data Sheet, M 280 and M 290 (2014)EOS GmbHarchived copyDMLS 316L Stainless Steel · Young's modulus (stiffness): typical, as built, horizontal (XY); EOSINT M280-400W / M290-400W, 316L_Surface 1.0, 20 µm (2014 sheet)
  4. 4
    EOS StainlessSteel 316L Material Data Sheet, FlexLine, M 290 (2016)EOS GmbHarchived copyDMLS 316L Stainless Steel · Density: part density (ISO 3369, not labelled min or typical), EOS M 290, 40 µm FlexLine
  5. 5
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7050-T7451 · Poisson's ratio: typical (handbook physical constant)
  6. 6
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyDMLS 316L Stainless Steel · Poisson's ratio: base material: austenitic stainless steels incl. 1.4404 (316L), design value
  7. 7
    316/316L Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 316L Stainless Steel · Thermal conductivity: base material: wrought 316/316L (Cleveland-Cliffs), at 100 °CDMLS 316L Stainless Steel · Specific heat: base material: wrought 316/316L (Cleveland-Cliffs), 0-100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS 316L Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 7050-T7451 stronger than DMLS 316L Stainless Steel?

DMLS 316L Stainless Steel is stronger: its yield strength is 530 MPa against 469 MPa for Aluminum 7050-T7451 (13%).

Which is lighter, Aluminum 7050-T7451 or DMLS 316L Stainless Steel?

Aluminum 7050-T7451 is lighter: 2,830 kg/m³ against 7,900 kg/m³ for DMLS 316L Stainless Steel.

Which is stiffer, Aluminum 7050-T7451 or DMLS 316L Stainless Steel?

DMLS 316L Stainless Steel is stiffer: Young's modulus 185 GPa against 70.3 GPa for Aluminum 7050-T7451, so the same part in DMLS 316L Stainless Steel deflects less under the same load.

Which is lighter for the same job, Aluminum 7050-T7451 or DMLS 316L Stainless Steel?

For the same stiffness or strength: Aluminum 7050-T7451 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7050-T7451DMLS 316L Stainless Steel
Stiff rod or tie (tension)lighter6% heavier
Stiff beam (bending)lighter1.72x heavier
Stiff panel or platelighter2.02x heavier
Strong rod or tielighter2.47x heavier
Strong beamlighter2.57x heavier
Strong panel or platelighter2.63x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7050-T7451 or DMLS 316L Stainless Steel?

DMLS 316L Stainless Steel stretches further before it breaks: 40% elongation at break against 11% for Aluminum 7050-T7451.

Thermal

Which conducts heat better, Aluminum 7050-T7451 or DMLS 316L Stainless Steel?

Aluminum 7050-T7451 conducts heat better: 157 W/m·K against 16.2 W/m·K for DMLS 316L Stainless Steel.

Which expands less with temperature?

DMLS 316L Stainless Steel expands less: 15.7 µm/m·K against 23.5 µm/m·K for Aluminum 7050-T7451.