Materials / Compare
Aluminum 7050-T7451 vs. Plastic POM/Acetal Compare Aluminum 7050-T7451 vs. Plastic POM/Acetal strength, stiffness, weight and thermal properties.
Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Aluminum 7050-T7451 Wrought Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Plastic POM/Acetal Bulk polymer (molded or machined) Mechanical Aluminum 7050-T7451 Plastic POM/Acetal Yield strength 469 MPa 6.8x stronger 69 MPa Ultimate tensile strength 524 MPa 7.59x stronger 69 MPa Compressive strength not sourced 124 MPa Flexural strength not sourced 99 MPa Elongation at break 11 % 75 % 6.82x more ductile Young's modulus (stiffness) 70.3 GPa 25.1x stiffer 2.8 GPa Density 2,830 kg/m³ 1,420 kg/m³ 1.99x lighter Strength to weight 166 kN·m/kg 3.41x higher 48.6 kN·m/kg Stiffness to weight 24.8 MN·m/kg 12.6x higher 1.97 MN·m/kg Poisson's ratio 0.33 0.35 Shear modulus 26.4 GPa 25.5x stiffer in shear 1.04 GPa Bulk modulus 68.9 GPa 22.2x higher 3.11 GPa Speed of sound 4,984 m/s 3.55x faster 1,404 m/s
1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 7050-T7451 Plastic POM/Acetal Stiffness against densityHigher and further left: stiffer for its weight 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 7050-T7451 Plastic POM/Acetal Strength against densityHigher and further left: stronger for its weight
Thermal Aluminum 7050-T7451 Plastic POM/Acetal Thermal conductivity 157 W/m·K 393x more heat through a fin 0.4 W/m·K Thermal expansion 23.5 µm/m·K 5.19x less mean 122 µm/m·K 100 mm part over a 50 °C swing 118 µm growth 5.19x less 610 µm growth Specific heat 860 J/kg·K average -18 to 100 °C 1,465 J/kg·K 1.7x higher Heats up and cools (diffusivity) 64.5 mm²/s 335x faster 0.192 mm²/s Thermal shock resistance 29,862 W/m 569x more resistant 52.5 W/m Melting point melting range 524–635 °C 175 °C Max service temperature not sourced HDT 1.8 MPa 125 °C
1k 10k 0.1 1 10 100 Density (kg/m³) Thermal conductivity (W/m·K) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 7050-T7451 Plastic POM/Acetal Thermal conductivity against densityHigher and further left: spreads more heat for its weight 0.1 1 10 100 10 100 Thermal conductivity (W/m·K) Thermal expansion (µm/m·K) Plastic PETG Plastic ABS Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 7050-T7451 Plastic POM/Acetal Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources 4 documents: Kaiser Aluminum, DuPont, U.S. Department of Defense
Aluminum 7050-T7451 7050-T7451 plate, Kaiser Aluminum sheet, coil & plate typical datasheet (longitudinal); Poisson from MIL-HDBK-5J
Plastic POM/Acetal DuPont Delrin 100 acetal homopolymer, Table 2 'Typical Properties of Delrin Acetal Resins' (ASTM methods), Delrin Design Guide Module III hosted on delrin.com 1 Alloy 7050 Sheet, Coil & Plate Technical Data Kaiser Aluminum archived copy Aluminum 7050-T7451 · Yield strength: typical, longitudinal, 0.2% offsetAluminum 7050-T7451 · Ultimate tensile strength: typical, longitudinalAluminum 7050-T7451 · Elongation at break: typical, longitudinalAluminum 7050-T7451 · Young's modulus (stiffness): typicalAluminum 7050-T7451 · Density: nominalAluminum 7050-T7451 · Thermal conductivity: typical, 20 °CAluminum 7050-T7451 · Thermal expansion: typical, mean 20-100 °CAluminum 7050-T7451 · Specific heat: typical, at 100 °CAluminum 7050-T7451 · Melting point: melting range2 Delrin Acetal Resin Design Guide, Module III DuPont archived copy Plastic POM/Acetal · Yield strength: typical (single ASTM D638 tensile strength)Plastic POM/Acetal · Ultimate tensile strength: typicalPlastic POM/Acetal · Compressive strength: compressive stress at 10% deformationPlastic POM/Acetal · Flexural strength: flexural yield strength, typicalPlastic POM/Acetal · Elongation at break: typicalPlastic POM/Acetal · Young's modulus (stiffness): typicalPlastic POM/Acetal · Poisson's ratio: typicalPlastic POM/Acetal · Thermal conductivity: typicalPlastic POM/Acetal · Thermal expansion: mean, 29 to 60 °CPlastic POM/Acetal · Specific heat: average -18 to 100 °C, Delrin acetal resins (not grade-specific)Plastic POM/Acetal · Melting point: crystalline melting pointPlastic POM/Acetal · Max service temperature: HDT 1.8 MPa (annealed)3 Delrin 100 Product Data Sheet DuPont Plastic POM/Acetal · Density: typical (DuPont product information for Delrin 100 NC010; 'The data listed here fall within the normal range of product properties')
4 MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003) U.S. Department of Defense Aluminum 7050-T7451 · Poisson's ratio: typical (handbook physical constant)
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions Mechanical Is Aluminum 7050-T7451 stronger than Plastic POM/Acetal? Aluminum 7050-T7451 is stronger: its yield strength is 469 MPa against 69 MPa for Plastic POM/Acetal (6.8x).
Which is lighter, Aluminum 7050-T7451 or Plastic POM/Acetal? Plastic POM/Acetal is lighter: 1,420 kg/m³ against 2,830 kg/m³ for Aluminum 7050-T7451.
Which is stiffer, Aluminum 7050-T7451 or Plastic POM/Acetal? Aluminum 7050-T7451 is stiffer: Young's modulus 70.3 GPa against 2.8 GPa for Plastic POM/Acetal, so the same part in Aluminum 7050-T7451 deflects less under the same load.
Which is lighter for the same job, Aluminum 7050-T7451 or Plastic POM/Acetal? For the same stiffness or strength: Aluminum 7050-T7451 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be Aluminum 7050-T7451 Plastic POM/Acetal Stiff rod or tie (tension) lighter 12.6x heavier Stiff beam (bending) lighter 2.51x heavier Stiff panel or plate lighter 47% heavier Strong rod or tie lighter 3.41x heavier Strong beam lighter 1.8x heavier Strong panel or plate lighter 31% heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Aluminum 7050-T7451 or Plastic POM/Acetal? Plastic POM/Acetal stretches further before it breaks: 75% elongation at break against 11% for Aluminum 7050-T7451.
Thermal Which conducts heat better, Aluminum 7050-T7451 or Plastic POM/Acetal? Aluminum 7050-T7451 conducts heat better: 157 W/m·K against 0.4 W/m·K for Plastic POM/Acetal.
Which expands less with temperature? Aluminum 7050-T7451 expands less: 23.5 µm/m·K against 122 µm/m·K for Plastic POM/Acetal.