Materials / Compare

Aluminum 7050-T7451 vs. Plastic UHMWPE

Compare Aluminum 7050-T7451 vs. Plastic UHMWPE strength, stiffness, weight and thermal properties.

Aluminum 7050-T7451Wrought
Plastic UHMWPEBulk polymer (molded or machined)
MechanicalAluminum 7050-T7451Plastic UHMWPE
Yield strength469MPa123.4x stronger20MPa2
Ultimate tensile strength524MPa143MPa2
Elongation at break11%1465%242.3x more ductile
Young's modulus (stiffness)70.3GPa1107x stiffer0.66GPa2
Density2,830kg/m³1930kg/m³23.04x lighter
Strength to weight166kN·m/kg7.71x higher21.5kN·m/kg
Stiffness to weight24.8MN·m/kg35x higher0.71MN·m/kg
Poisson's ratio0.333not sourced
Shear modulus26.4GPanot sourced
Bulk modulus68.9GPanot sourced
Speed of sound4,984m/s5.92x faster842m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Plastic UHMWPE
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Plastic UHMWPE
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7050-T7451Plastic UHMWPE
Thermal conductivity157W/m·K1393x more heat through a fin0.4W/m·K4
Thermal expansion23.5µm/m·K18.51x less200µm/m·K4
100 mm part over a 50 °C swing118µm growth8.51x less1,000µm growth
Specific heat860J/kg·K1not sourced
Heats up and cools (diffusivity)64.5mm²/snot sourced
Thermal shock resistance29,862W/mnot sourced
Melting pointmelting range524–635°C1DSC 10 K/min130–138°C2
Max service temperaturenot sourced80°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Plastic UHMWPE
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7050-T7451Plastic UHMWPE
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Celanese, U.S. Department of Defense
Aluminum 7050-T7451
7050-T7451 plate, Kaiser Aluminum sheet, coil & plate typical datasheet (longitudinal); Poisson from MIL-HDBK-5J
Plastic UHMWPE
Celanese GUR 4120 (avg. molecular weight 4.7x10^6 g/mol), typical values on compression-molded specimens; CTE and thermal conductivity from Celanese's generic UHMWPE guide (grade not named)
  1. 1
    Alloy 7050 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7050-T7451 · Yield strength: typical, longitudinal, 0.2% offsetAluminum 7050-T7451 · Ultimate tensile strength: typical, longitudinalAluminum 7050-T7451 · Elongation at break: typical, longitudinalAluminum 7050-T7451 · Young's modulus (stiffness): typicalAluminum 7050-T7451 · Density: nominalAluminum 7050-T7451 · Thermal conductivity: typical, 20 °CAluminum 7050-T7451 · Thermal expansion: typical, mean 20-100 °CAluminum 7050-T7451 · Specific heat: typical, at 100 °CAluminum 7050-T7451 · Melting point: melting range
  2. 2
    GUR UHMW-PE Overview (GUR-015)CelanesePlastic UHMWPE · Yield strength: typical, tensile stress at yield ISO 527, 50 mm/minPlastic UHMWPE · Ultimate tensile strength: typical, tensile stress at break ISO 527, 50 mm/minPlastic UHMWPE · Elongation at break: typical, nominal elongation at break ISO 527Plastic UHMWPE · Young's modulus (stiffness): typical, tensile modulus ISO 527, 1 mm/minPlastic UHMWPE · Density: typicalPlastic UHMWPE · Melting point: DSC 10 K/minPlastic UHMWPE · Max service temperature: recommended max constant operating temperature
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7050-T7451 · Poisson's ratio: typical (handbook physical constant)
  4. 4
    GUR UHMW-PE Polymer Guide (GUR-003)Celanesearchived copyPlastic UHMWPE · Thermal conductivity: typical, unfilled (narrative value, generic Celanese UHMWPE)Plastic UHMWPE · Thermal expansion: typical, 20 to 100 °C (generic Celanese UHMWPE)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 7050-T7451 stronger than Plastic UHMWPE?

Aluminum 7050-T7451 is stronger: its yield strength is 469 MPa against 20 MPa for Plastic UHMWPE (23.4x).

Which is lighter, Aluminum 7050-T7451 or Plastic UHMWPE?

Plastic UHMWPE is lighter: 930 kg/m³ against 2,830 kg/m³ for Aluminum 7050-T7451.

Which is stiffer, Aluminum 7050-T7451 or Plastic UHMWPE?

Aluminum 7050-T7451 is stiffer: Young's modulus 70.3 GPa against 0.66 GPa for Plastic UHMWPE, so the same part in Aluminum 7050-T7451 deflects less under the same load.

Which is lighter for the same job, Aluminum 7050-T7451 or Plastic UHMWPE?

For the same stiffness or strength: Aluminum 7050-T7451 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7050-T7451Plastic UHMWPE
Stiff rod or tie (tension)lighter35x heavier
Stiff beam (bending)lighter3.39x heavier
Stiff panel or platelighter1.56x heavier
Strong rod or tielighter7.71x heavier
Strong beamlighter2.69x heavier
Strong panel or platelighter1.59x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7050-T7451 or Plastic UHMWPE?

Plastic UHMWPE stretches further before it breaks: 465% elongation at break against 11% for Aluminum 7050-T7451.

Thermal

Which conducts heat better, Aluminum 7050-T7451 or Plastic UHMWPE?

Aluminum 7050-T7451 conducts heat better: 157 W/m·K against 0.4 W/m·K for Plastic UHMWPE.

Which expands less with temperature?

Aluminum 7050-T7451 expands less: 23.5 µm/m·K against 200 µm/m·K for Plastic UHMWPE.

Related comparisons